Нагряване на стоманени дюбели преди коване
  • Нагряване на стоманени дюбели преди коване

Снимките са само с информационна цел. Вижте спецификацията на продукта

please use latin characters

Производител: Ambrell

Нагряване на стоманени дюбели преди коване

Preheating for Forging of Steel Pins


Objective: To heat magnetic steel pins (spokes) for forging on a rim without heat treating and weakening the rim. Previously, a torch was utilized and the heating time was 20 seconds.


Frequency: 294 kHz


Equipment:
  • Ambrell EASYHEATTM 8310 LI, 10 kW induction heating system, equipped with a remote workhead containing one 1 μF capacitor;
  • A helical induction heating coil designed and developed specifically for this application.

Material: 9/16” (14 mm) steel pins.


Temperature: 2000 °F (1093 °C)


Process:

A single position three-turn helical coil was used, and the part was placed under the coil. The part was heated to the desired temperature within just seven seconds.


Benefits:
  • Fast, precise heating of the pin – 2 minutes and 36 seconds were saved on heating all of the rim’s pins when compared to using a torch;
  • The rim was not heated, which maintained its strength and durability;
  • Energy was saved due to the reduction in heating time;
  • There is more repeatability with induction when compared to using a torch.

Изпратете запитване

Интересувате ли се от този продукт? Имате ли нужда от допълнителна информация или индивидуални цени?

Свържете се с нас
ПОИСКАЙТЕ ПРОДУКТА close
Благодарим ви, че изпратихте съобщението си. Ние ще отговорим възможно най-скоро.
ПОИСКАЙТЕ ПРОДУКТА close
Преглед

Добави към списъка с желания

Трябва да сте влезли

Preheating for Forging of Steel Pins


Objective: To heat magnetic steel pins (spokes) for forging on a rim without heat treating and weakening the rim. Previously, a torch was utilized and the heating time was 20 seconds.


Frequency: 294 kHz


Equipment:
  • Ambrell EASYHEATTM 8310 LI, 10 kW induction heating system, equipped with a remote workhead containing one 1 μF capacitor;
  • A helical induction heating coil designed and developed specifically for this application.

Material: 9/16” (14 mm) steel pins.


Temperature: 2000 °F (1093 °C)


Process:

A single position three-turn helical coil was used, and the part was placed under the coil. The part was heated to the desired temperature within just seven seconds.


Benefits:
  • Fast, precise heating of the pin – 2 minutes and 36 seconds were saved on heating all of the rim’s pins when compared to using a torch;
  • The rim was not heated, which maintained its strength and durability;
  • Energy was saved due to the reduction in heating time;
  • There is more repeatability with induction when compared to using a torch.