Călirea vârfurilor din oțel ale pumnilor de mână
  • Călirea vârfurilor din oțel ale pumnilor de mână

Fotografiile au doar scop informativ. Vizualizați specificațiile produsului

please use latin characters

Producător: Ambrell

Călirea vârfurilor din oțel ale pumnilor de mână

Hardening the end of steel hand-held marking stamps


Objective: To harden various size ends of hand held marking stamps. The area to be hardened is 3/4” (19mm) up the shank.


Equipment:
  • Ambrell 30 kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF;
  • An induction heating coil designed and developed specifically for this application.

Material: Steel stamps 1/4” (6.3mm), 3/8” (9.5mm), 1/2” (12.7mm) and 5/8” (15.8mm) square


Temperature: 1550 ºF (843 ºC)



Frequency: 99 kHz


Process:

A two turn channel coil is used to cover the range of steel stamps being heated. The 5/8” steel stamp is heated for 60 seconds to reach 1550 ºF (843 ºC) and the desired hardness. Smaller parts will also heat easily.


Benefits:
  • Faster process time and production rates;
  • Hands-free heating that involves no operator skill for manufacturing;
  • Controlled precise application of heat.

Trimite o cerere

Sunteți interesat de acest produs? Aveți nevoie de informații suplimentare sau de prețuri individuale?

Contactează-ne
CERETI PRODUSUL close
Vă mulțumim că ați trimis mesajul dvs. Vom răspunde cât mai curând posibil.
CERETI PRODUSUL close
Naviga

Adaugă la lista de dorințe

trebuie să fii logat

Hardening the end of steel hand-held marking stamps


Objective: To harden various size ends of hand held marking stamps. The area to be hardened is 3/4” (19mm) up the shank.


Equipment:
  • Ambrell 30 kW induction heating system, equipped with a remote workhead containing eight 1.0μF capacitors for a total of 2.0μF;
  • An induction heating coil designed and developed specifically for this application.

Material: Steel stamps 1/4” (6.3mm), 3/8” (9.5mm), 1/2” (12.7mm) and 5/8” (15.8mm) square


Temperature: 1550 ºF (843 ºC)



Frequency: 99 kHz


Process:

A two turn channel coil is used to cover the range of steel stamps being heated. The 5/8” steel stamp is heated for 60 seconds to reach 1550 ºF (843 ºC) and the desired hardness. Smaller parts will also heat easily.


Benefits:
  • Faster process time and production rates;
  • Hands-free heating that involves no operator skill for manufacturing;
  • Controlled precise application of heat.