Objective: To heat a magnetic steel gear for a shrink fitting application; they’re looking to replace an oven that takes over two hours to heat the part to temperature.
Frequency: 180 kHz
Material: Magnetic steel gear, 2” (55 mm) ID, 12.5” (318 mm) OD
Temperature: 550 °F ()
A custom-designed single position multiple-turn pancake coil was built to generate the required heating for this shrink fitting application. Initial tests were conducted to optimize the power delivered to the part. Temperature indicating paint was then applied to the part, which dissolves when the part reaches the target temperature.
It was observed that it took 45 minutes to heat the sample to temperature. The coil can be placed beneath the gear to allow oil to burn off without condensing on the coil.
Вы заинтересованы в этом продукте? Вам нужна дополнительная информация или индивидуальные расценки?
Вы должны быть зарегистрированы
Objective: To heat a magnetic steel gear for a shrink fitting application; they’re looking to replace an oven that takes over two hours to heat the part to temperature.
Frequency: 180 kHz
Material: Magnetic steel gear, 2” (55 mm) ID, 12.5” (318 mm) OD
Temperature: 550 °F ()
A custom-designed single position multiple-turn pancake coil was built to generate the required heating for this shrink fitting application. Initial tests were conducted to optimize the power delivered to the part. Temperature indicating paint was then applied to the part, which dissolves when the part reaches the target temperature.
It was observed that it took 45 minutes to heat the sample to temperature. The coil can be placed beneath the gear to allow oil to burn off without condensing on the coil.